Cause analysis of defects in valve casting during production

Time:2018-11-24
1. The stomataThis is a small cavity formed by the gas that cannot be escaped from the metal during solidification. Its inner wall is smooth and contains gas, and it has a high reflectivity to ultrasonic wave.

1. The stomata

This is a small cavity formed by the gas that cannot be escaped from the metal during solidification. Its inner wall is smooth and contains gas, and it has a high reflectivity to ultrasonic wave. However, because it is basically spherical or ellipsoidal, it is also a point defect, which affects its reflected amplitude. After forging or rolling, the pores in ingots are compressed into area defects, which are favorable for ultrasonic detection.

2. Shrinkage cavity and porosity

When the casting or ingot is cooled and solidified, the volume should shrink, and the final solidified part can not be replaced by liquid metal, thus forming a void defect. Large and concentrated voids are called shrinkage holes, and small and dispersed voids are called loose. They are generally located in the last solidified part of the ingot or casting center. The inner wall is rough, and there are many impurities and small pores around them. Due to the law of thermal expansion and cold shrinkage, shrinkage holes are inevitable, but they have different shapes, sizes and positions with different processing methods. When they extend to casting or ingot body, they become defects. If the shrinkage cavity is not removed and brought into the forgings, the ingot will become the residual shrinkage cavity (shrinkage cavity residual, residual shrinkage pipe).

3. The slag

Slag inclusion defect is formed when the slag or refractory material on the furnace body breaks off and enters the liquid metal during the melting process and gets involved in the casting or ingot body during pouring. Slag inclusion usually does not exist in a single, often dense state or dispersed in different depths, it is similar to the volume type of defects but often have a certain degree of linearity.

4. The inclusions

Reaction products (such as oxides, sulphides, etc.) in the melting process - non-metallic inclusion, or some components of the metal components of the additive material is not completely melted and residual metal inclusion, such as high density, high melting point components - tungsten, molybdenum, etc.

5. Segregation

The segregation of castings or ingots mainly refers to the composition segregation caused by uneven distribution of components in the smelting process or the melting process of metals. The mechanical properties of regions with segregation are different from the mechanical properties of the entire metal matrix, and the difference beyond the allowable standard range becomes a defect.

6. Casting cracks

Of casting cracks is mainly due to the metal cooling solidification contraction caused by the stress exceeds the limit of material strength, it is related to the shape of the casting design and casting process, also with some high content of impurities in the metal materials caused by cracking sensitivity about (such as sulfur content high brittleness, high phosphorus content with cold brittleness, etc.). Axial crystal cracks may also occur in ingots. If they cannot be forged together in the subsequent open-billet forging, they will remain in the forgings and become internal cracks in the forgings.

7. Cold insulation

This is a kind of stratification peculiar to the casting defects, mainly related to the casting casting process design, when it is pouring liquid metal, due to interruption of splash, double wave, pouring, or from two different directions (or more) metal flow meet, because the liquid metal semi-solid film on the casting cooling formation on the surface of the body and form a membrane of the area of defects.

8. Skull patch

This is when the steel from ladle to mold casting ingot, because pouring interrupt, pause, first poured into the surface of the liquid metal rapidly cooled in air oxidation film formation, continuing pouring new pouring into the liquid metal to break through its turn into steel ingot and formed a kind of stratification (area) defect, it is not in the subsequent breakdown of ingot forging forging close to eliminate.

anisotropy

When casting or steel ingot is cooled and solidified, the cooling speed from the surface to the center is different, so different crystal structures will be formed, which is manifested as anisotropy of mechanical properties, and also leads to anisotropy of acoustic properties, that is, there are different sound velocities and sound attenuation from the center to the surface. The existence of this anisotropy will have a bad effect on the size and position of casting defects in ultrasonic testing.

主站蜘蛛池模板: 成人a级网站| 超碰97人人做人人爱亚洲 | 中文字幕免费不卡视频 | 99999久久久久9国产精品 | 在线观看国产精品一区二区 | 亚洲精品中 | 中文字幕影视免费观看 | 国产精品成人在线观看 | 日韩国产成人精品视频人 | 国产高清乱理伦片中文小说 | 男人午夜av | 国产亚洲欧美日韩综合另类 | 一级免费看视频 | 久久丝袜脚交足黄网站免费 | 亚洲中文成人中文字幕 | 国产不卡视频在线播放 | 国产精品久久9 | 国精产品久久 | 国产黄色片一级 | 2018国产精品视频麻 | 女人体1963午夜免费视频软件 | 国产精品午夜爆乳美女视频 | 高清亚洲| 综合一区在线 | 国产精品久久久久无码A孕妇 | 国产成人乱色视频网站 | 日韩一级大片在线 | 久久一区二区免费视频 | 欧美77| 91久久香蕉 | 国产精品成人久久久久久久 | 97色伦欧美一区二区日韩 | 精品国产乱码久久久久久老虎 | 亚洲精品无码人妻无码 | 亚洲一区二区三区四区在线观看 | 最近的中文字幕在线看视频 | 少妇高潮一区二区三区99小说 | 国产欧洲精品色在线 | 裸体精品bbbbbbbbb美国 | 欧美一级特黄aa大片 | a级黄色网址 |